Steel Grade Equivalents: S235, S275 and S355 vs ASTM, JIS, GB and Other Standards

Published November 2026  ·  9 min read  ·  Technical Reference  ·  Structural Steel

A drawing from Germany specifies S355J2, the supplier quotes ASTM A572 Grade 50, and the client's old standard still says St52-3. Are they the same steel? Close, but not exactly. This guide gives a cross-reference of structural steel grades across European, American, Japanese, Chinese, Indian, Canadian, Australian and Russian standards. It also explains the differences that matter when you substitute one grade for another, and includes a grade equivalent finder.

Quick answers
• S235JR ≈ ASTM A36 ≈ JIS SS400 ≈ GB Q235B ≈ old DIN St37-2.
• S275JR ≈ ASTM A572 Grade 42 ≈ old BS 4360 43A.
• S355J2 ≈ ASTM A572 Grade 50 / A992 ≈ JIS SM490B ≈ GB Q355B ≈ old DIN St52-3.
• The number in an EN grade is the minimum yield strength in MPa for thin sections. The letters show the impact test temperature.
• "Equivalent" means similar strength, not identical. Toughness, chemistry and thickness limits can differ.

How to Read a European Steel Grade

European structural grades follow EN 10027-1. Take S355J2+N as an example:

PartMeaning
SStructural steel
355Minimum yield strength in MPa for thicknesses up to 16 mm. It decreases for thicker products.
J2Impact energy of at least 27 J at −20 °C. JR = +20 °C, J0 = 0 °C, J2 = −20 °C. K2 = 40 J at −20 °C.
+NDelivery condition: normalised or normalised rolled. +AR = as rolled, +M = thermomechanically rolled (EN 10025-4).

Hollow sections add an "H" (S355J2H), and coated sheet uses "GD" (S350GD). See our guides to hollow sections and galvanized steel grades.

Grade Equivalent Finder

Grades are grouped by similar minimum yield strength. Values are for thin products (typically up to 16 mm). Check the full standard for thicker sections and other requirements.

Structural Steel Equivalents Table

Approx. 235–250 MPa class

GradeStandardRegionMin. yield (MPa)Tensile (MPa)Impact test
S235JREN 10025-2Europe235360–51027 J at +20 °C
S235J2EN 10025-2Europe235360–51027 J at −20 °C
ASTM A36ASTM A36USA250400–550Not required unless specified
SS400JIS G3101Japan245400–510Not specified
SM400BJIS G3106Japan245400–51027 J at 0 °C
Q235BGB/T 700China235370–50027 J at +20 °C
E250IS 2062India250min. 410Depends on quality A/BR/B0/C
St3spGOST 380Russia/CIS245370–480Depends on category
St37-2DIN 17100 (withdrawn)Old German235340–470Old name of S235JR

Approx. 275–300 MPa class

GradeStandardRegionMin. yield (MPa)Tensile (MPa)Impact test
S275JREN 10025-2Europe275410–56027 J at +20 °C
S275J2EN 10025-2Europe275410–56027 J at −20 °C
ASTM A572 Gr. 42ASTM A572USA290min. 415Not required unless specified
300WCSA G40.21Canada300450–620Not required for W
Grade 300AS/NZS 3679.1Australia300min. 440L0 grades tested at 0 °C
43ABS 4360 (withdrawn)Old British275430–580Old name ~S275JR

Approx. 345–355 MPa class

GradeStandardRegionMin. yield (MPa)Tensile (MPa)Impact test
S355JREN 10025-2Europe355470–63027 J at +20 °C
S355J2EN 10025-2Europe355470–63027 J at −20 °C
S355K2EN 10025-2Europe355470–63040 J at −20 °C
ASTM A572 Gr. 50ASTM A572USA345min. 450Not required unless specified
ASTM A992ASTM A992USA345min. 450Not required unless specified; max. yield 450 MPa
SM490BJIS G3106Japan325490–61027 J at 0 °C
Q355BGB/T 1591China355470–63034 J at +20 °C
E350IS 2062India350min. 490Depends on quality
350WCSA G40.21Canada350450–650Not required for W
Grade 350AS/NZS 3679.1Australia350min. 480L0 grades tested at 0 °C
09G2SGOST 19281Russia/CIS345min. 490Tested at −40 °C in higher categories
St52-3DIN 17100 (withdrawn)Old German355490–630Old name of S355J2
50DBS 4360 (withdrawn)Old British355490–640Old name ~S355K2

Approx. 450–460 MPa class

GradeStandardRegionMin. yield (MPa)Tensile (MPa)Impact test
S460MEN 10025-4Europe460540–72040 J at −20 °C
ASTM A572 Gr. 65ASTM A572USA450min. 550Not required unless specified
SM570JIS G3106Japan460570–72047 J at −5 °C
Q460CGB/T 1591China460550–72034 J at 0 °C

Minimum yield strength for the thinnest thickness range; tensile strength ranges as given in the standards for common thicknesses. Values can differ between editions of a standard. This table is a guide for comparison, not a substitute for the specification.

Old Names You Will Still See

Many drawings and machines still carry withdrawn designations. The most common conversions are:

Old designationOld standardCurrent EN gradeMaterial number
St37-2DIN 17100S235JR1.0038
St37-3DIN 17100S235J21.0117
St44-2DIN 17100S275JR1.0044
St52-3DIN 17100S355J21.0577 (+N)
Fe 360 BEN 10025:1990S235JR1.0038
Fe 510 D1EN 10025:1990S355J21.0577
43A / 43CBS 4360S275JR / S275J01.0044 / 1.0143
50B / 50DBS 4360S355JR / S355K21.0045 / 1.0596

Why "Equivalent" Is Not "Identical"

Grades with the same strength can still behave differently. Check these five points before you accept a substitute:

Impact toughness

S355J2 guarantees 27 J at −20 °C. ASTM A572 Grade 50 and A36 have no impact test unless a supplementary requirement is ordered. For cold climates or dynamic loads, this difference matters.

Thickness dependence

EN grades lose yield strength in steps as thickness increases (S355 drops to 345 MPa above 16 mm). Other standards use different steps, so compare at the actual thickness.

Chemistry and weldability

Maximum carbon, CEV and impurity limits differ. A grade can match in strength and still need a different welding procedure. See our mill test certificate guide for the CEV check.

Upper yield limit

ASTM A992 limits the maximum yield strength and the yield-to-tensile ratio for seismic design. Most EN grades have no maximum yield. A stronger-than-specified steel is not always acceptable.

Documents and marking

CE marking under EN 1090 requires EN-certified products with 3.1 certificates. A steel that only meets an ASTM grade may not be acceptable on an EU project, and vice versa.

Dual certification: Many mills, including Turkish mills, produce beams and plates that meet two standards at once, for example S355J2 + ASTM A572 Grade 50 or S355JR + A992. The mill test certificate then lists both grades and the test results for each. If you supply projects in different markets, ask for dual-certified material.

Substituting a Grade: A Practical Checklist

  • Compare yield and tensile strength at the actual thickness, not only the grade name.
  • Compare impact requirements: test temperature, energy and specimen direction.
  • Check chemistry and CEV against the welding procedure qualified for the project.
  • Check special requirements: through-thickness properties (Z grades), maximum yield, galvanizability (silicon and phosphorus).
  • Check the documents: certificate type (EN 10204 3.1 or 3.2), CE marking, and project approval.
  • Get written approval from the structural engineer or the client before you substitute.

Sourcing Structural Steel from Türkiye

Turkish mills produce structural sections, plates and hollow sections to EN 10025 and EN 10219, and many also certify to ASTM, JIS or other national standards for export markets. This makes Türkiye a convenient source for projects in Europe, the Middle East, Africa and the Americas. See our structural steel sections, and the size tables for HEA/HEB and IPE beams.

Frequently Asked Questions

What is the ASTM equivalent of S355J2?

The nearest ASTM equivalent is A572 Grade 50, or A992 for wide-flange beams. Both have a minimum yield strength of 345 MPa. S355J2 also guarantees 27 J impact energy at −20 °C, which the ASTM grades only provide if a supplementary impact test is ordered.

Is S235JR the same as ASTM A36?

They are close but not identical. S235JR has a minimum yield strength of 235 MPa and A36 has 250 MPa. S235JR requires an impact test at +20 °C, while A36 has no standard impact requirement. They are often treated as equivalent for general structural work.

What is the Chinese equivalent of S355?

The Chinese equivalent is Q355 to GB/T 1591, which replaced the older Q345. Q355B is tested at +20 °C, Q355C at 0 °C and Q355D at −20 °C, so Q355D is the closest match to S355J2.

What is the JIS equivalent of S235 and S355?

JIS SS400 or SM400 is broadly equivalent to S235, and SM490 is broadly equivalent to S355. Note that SS400 has no limits on carbon and impact properties, while the SM grades are weldable structural steels with tighter requirements.

What is St52-3 called today?

St52-3 from the old DIN 17100 corresponds to S355J2 (material number 1.0577) under EN 10025-2. St37-2 corresponds to S235JR.

Can I replace S355 with ASTM A572 Grade 50 on a European project?

Only with approval. The strength is similar, but the impact toughness, chemistry limits and certification differ, and CE marking under EN 1090 normally requires EN-certified material. Dual-certified steel that meets both standards avoids the problem.

Need steel to a specific standard?

Send your grade, standard and quantities. Steeling.net returns offers from Turkish mills for EN, ASTM and dual-certified structural steel with 3.1 certificates. There are no fees for buyers.

Get a Free Quote →