Press Brake Bending Design Guide: Bend Radius, Minimum Flange, K-Factor and Tonnage

Published November 2026  ·  10 min read  ·  Design Guide  ·  Sheet Metal

Most problems with bent sheet metal parts are designed in, not made in: a flange too short for the die, a hole that distorts because it sits too close to the bend, a radius the material cannot take without cracking, or a flat pattern calculated with the wrong K-factor. This guide gives the practical rules press brake shops use — V-die selection, inside radius, minimum flange length, hole distances, bend relief, springback, K-factor and bending force — and a calculator that applies them to your part.

Quick answers
• V-die opening: about 6–8 × thickness for thin sheet (t ≤ 3 mm), about 8–10 × t for 3–15 mm and 10–12 × t for thicker plate.
• Inside radius (air bending): roughly 15–17% of the V opening for mild steel, about 20–22% for stainless steel and 13–15% for soft aluminium.
• Minimum flange length: about 0.7 × V opening (measured to the outside of the bend). Shorter flanges fall into the die.
• Holes near bends: keep hole edges at least about 2.5 × t + inside radius from the bend line, or they will distort.
• K-factor: about 0.33 for sharp bends, 0.40–0.45 for typical air bending and up to 0.5 for large radii.
• Bending force (90° air bend): F (kN) ≈ 1.33 × L × t² × Rm / (V × 1000), with L, t, V in mm and tensile strength Rm in MPa.

Air Bending, Bottoming and Coining

Almost all modern CNC press brake work is air bending: the punch pushes the sheet into a V-die without forcing it to the bottom, and the bend angle is set by the punch depth. Air bending needs the least force and one die set covers many angles, but the inside radius is defined by the V opening, not by the punch, and springback must be compensated by the CNC control. Bottoming presses the sheet against the die faces for better angle repeatability, at roughly two to three times the force. Coining stamps the punch tip into the material, needs many times more force and is rarely used today except for very thin, precise parts. Unless your drawing says otherwise, assume air bending.

Choosing the V-Die and Inside Radius

In air bending, the V-die opening controls the inside radius, the minimum flange and the force. A wider die gives a larger radius and lower force; a narrower die gives a tighter radius, shorter possible flanges and higher force.

Thickness t (mm)V-die (mm)Inside radius ≈ (mm)Min. flange ≈ (mm)Force (kN/m)Force (t/m)
0.861.04606.1
181.36707.1
1.5121.9810510.7
2162.61114014.2
2.5203.21417517.8
3243.81720921.4
4355.62425526.0
5406.42834935.6
6508.03540241.0
8609.64259660.7
108012.85669871.2
1210016.07080482.0
1512520.0881005102.5
2020032.01401117113.9

Typical values for mild steel (Rm about 400–450 MPa), 90° air bending, rounded to common die sizes. Force per metre of bend length. Actual dies vary by shop; stainless steel needs about 1.5 times the force of mild steel, aluminium about half.

Specify radii the shop can make. If the drawing calls for an inside radius that does not match a standard V-die (for example r = 1 mm in 6 mm plate), the shop will either use a special tool, bend in several steps (bump bending) or ask you to change the design. Where the exact radius is not functional, write "inside radius per standard tooling" or give a radius range.

Minimum Bend Radius by Material

Bending too tightly cracks the outside of the bend, especially in high-strength steels, hard aluminium tempers and when bending parallel to the rolling direction.

MaterialTypical minimum inside radiusNotes
Mild steel (S235, DC01, DX51D)about 1 × t (often less in thin sheet)Bends easily; galvanized coatings may crack at very tight radii
Structural steel S355about 1–1.5 × tBend across the rolling direction for thick plate
High-strength steel (S500MC–S700MC)about 1.5–2.5 × t or moreCheck EN 10149-2 or the mill's bending data; higher springback
Wear plate (e.g. 400 HBW)about 3–4 × tFollow the plate producer's bending guide strictly
Stainless steel 304 / 316about 1–2 × tHigher force and springback than mild steel
Aluminium 5754 / 5083 (H22, H32)about 1–2 × tGood bendability
Aluminium 6061-T6 / 6082-T6about 2–4 × t or moreProne to cracking; bend in T4 or annealed condition if a tight radius is needed

Guide values only. The applicable material standard and supplier data take precedence.

Design Rules for Bent Parts

  • Minimum flange: at least about 0.7 × V opening to the outside of the bend. For 2 mm steel in a 16 mm die, that is about 11 mm.
  • Holes and slots near bends: keep the hole edge at least 2.5 × t + inside radius from the bend line. If you cannot, add a relief slot along the bend line or cut the hole after bending.
  • Bend relief: where a bend ends inside the sheet, add a relief cut about t wide (at least 1 mm) and at least t + inside radius deep to prevent tearing.
  • Flanges near each other: leave enough space between bends for the punch; U-channels with a flange shorter than the punch clearance need gooseneck tools or a different design.
  • Rolling direction: for high-strength steel, thick plate and hard aluminium, bend across the rolling direction where possible, and mark it on the drawing if critical.
  • Consistent radii: use the same inside radius and thickness throughout a part to avoid tool changes.
  • Dimensioning: dimension bent parts to the outside or inside of flanges consistently, from a functional datum, and avoid tight tolerances chained across several bends.
  • Tolerances: typical press brake tolerances are about ±0.5° to ±1° on angles and about ±0.2–0.5 mm on flange lengths for thin sheet, larger on thick plate.

K-Factor, Bend Allowance and Flat Pattern Length

When sheet is bent, the outside stretches and the inside compresses. The neutral axis, which keeps its length, moves towards the inside of the bend. The K-factor is the ratio of the neutral axis position to the thickness (K = tn / t). It decides how long the flat blank must be.

QuantityFormula
Bend allowance (arc length of neutral axis)BA = π × A / 180 × (r + K × t)
Outside setback (for angle A)OSSB = tan(A / 2) × (r + t)
Bend deductionBD = 2 × OSSB − BA
Flat length of an L-partLflat = a + b − BD (a, b = outside flange dimensions)
Bend conditionTypical K-factor
Inside radius smaller than thickness (r < t)about 0.33
Air bending, r about 1–3 × t (most parts)about 0.40–0.45
Large radius (r > 3 × t)about 0.45–0.50

CAD systems use a default K-factor or bend table. If your parts must fit precisely, ask the manufacturer for their bend deduction values for your material and thickness, or let them unfold the 3D model with their own tables — send STEP files as described in our RFQ guide for custom metal parts.

Press Brake Bending Calculator

Enter the material, thickness and bend length. The calculator suggests a V-die, estimates the inside radius, minimum flange and force, and calculates the flat length of an L-shaped part for a 90° bend.

Approximate air-bending values for planning and quote comparison. Final tooling, radius and flat lengths are set by the manufacturer.

Springback and Angle Accuracy

After the punch retracts, the sheet springs back by a few degrees. Mild steel typically springs back around 1–2°, stainless steel around 2–4°, and high-strength steels and some aluminium alloys more. Modern CNC press brakes compensate automatically, and machines with angle measurement systems correct each bend, which matters for long parts, high-strength materials and tight angle tolerances. If your parts need angles better than about ±0.5°, say so in the RFQ, because it affects the choice of machine.

Press Brake Capacity in Türkiye

Türkiye is a major press brake producer (Durma, Ermaksan, Baykal and others) and has a dense network of sheet metal subcontractors that combine laser cutting, CNC bending, welding and powder coating under one roof. Steeling.net's partner manufacturers bend sheet and plate on CNC press brakes with bending lengths up to about 3,000–4,000 mm, and heavy fabricators handle plate up to about 50 mm thick. Learn more about our CNC bending service, check cutting limits in our fiber laser thickness chart, or estimate part weight with the steel weight calculator.

Frequently Asked Questions

What V-die should I use for sheet metal bending?

A common rule is a V-die opening of about 6–8 times the material thickness for sheet up to 3 mm, about 8–10 times for 3–15 mm and 10–12 times for thicker plate. For example, 2 mm mild steel is usually bent in a 12–16 mm V-die and 6 mm plate in a 50 mm V-die.

What is the minimum flange length for press brake bending?

The minimum flange length is roughly 0.7 times the V-die opening, measured to the outside of the bend. A 2 mm sheet bent in a 16 mm die needs a flange of at least about 11 mm; shorter flanges slip into the die and need special tooling or a design change.

What inside bend radius does air bending produce?

In air bending the inside radius is set by the V-die opening, not by the punch. It is roughly 15–17% of the V opening for mild steel, about 20–22% for stainless steel and about 13–15% for soft aluminium. A 16 mm V-die therefore gives an inside radius of about 2.5 mm in mild steel.

What K-factor should I use for sheet metal?

For typical air bending with an inside radius of 1–3 times the thickness, a K-factor of about 0.40–0.45 is common. Use about 0.33 for sharp bends where the radius is smaller than the thickness and up to 0.5 for large radii. For precise parts, use the manufacturer's bend deduction tables.

How do I calculate press brake tonnage?

For a 90° air bend, force in kN is approximately 1.33 × bend length × thickness² × tensile strength / (V-die opening × 1000), with lengths in mm and tensile strength in MPa. For example, 3 mm mild steel (420 MPa) in a 24 mm die needs about 210 kN, or roughly 21 tonnes, per metre of bend.

How far should holes be from a bend?

Keep the edge of a hole at least about 2.5 times the thickness plus the inside radius away from the bend line. Closer holes stretch into ovals during bending. If that is not possible, add a relief slot along the bend or cut the holes after bending.

Need bent sheet metal parts?

Send your drawings and STEP files, material, thickness and quantities. Steeling.net matches your parts with Turkish manufacturers that combine laser cutting, CNC bending, welding and finishing. There are no fees for buyers.

Request a Quote →